Entanglement Molecular Weights

Polymer/ Entanglement Weight Me1
(g/mol)
Poly(4-tert-butylphenyl methacrylate) 64850
Poly(4-tert-butylstyrene) 21675
Poly(Bisphenol A carbonate), PC 2510
Poly(Bisphenol-A diglycidyl ether), PDGEBA 1570
Poly(bisphenol A isophthalate) 2450
Poly(Bisphenol A terephthalate) 1395
PoIy(1,2-butadiene) 3710
Poly(1,3-butadiene) 2480
Poly(1,4-butadiene) 2380
Poly(1-butene), PB-1 12260
Poly(caprolactam), Nylon 6 2490
Poly(2-chlorophenyl methacrylate) 52040
Poly(cyclohexyl methacrylate), PCHMA 34690
Poly(cyclohexylethene) 44120
Poly(decyl methacrylate) 61120
Poly(2,6-dimethyl-p-phenylene oxide), PPO 3570
Poly(dodecyl methacrylate) 112050
Poly(ethyl acrylate), PEA 8180
Poly(ethylene glycol), PEG 1850
Poly(ethylene terephthalate), PET 1450
Poly(ethylene), PE 1160
Poly(hexamethylene adipamide), Nylon 6,6 2010
Poly(hexane-1,6-diyl isophthalamide) 1940
Poly(hexyl methacrylate) 33450
Poly(isobutene) 7935
Poly(isopentene) 6580
Poly(methyl acrylate), PMA 10035
Poly(1-methyl-1-butenylene) 4085
Poly(methyl methacrylate), PMMA 11325
Poly(octadecyl methacrylate) 225140
Poly(phenyl methacrylate) 45440
Poly(propylene) 4595
Poly(tert-butyl methacrylate) 28260
Poly(tetradecyl methacrylate) 92440
Poly(tetrafluoroethene), PTFE 4650
Poly(tetramethyl Bisphenol A carbonate) 3420
Poly(tetramethyl bisphenol A isophthalate) 3970
Poly(vinyl acetate) 9680
Poly(vinyl chloride), PVC 5410
Poly(α-methylstyrene)  16370
Polyacetal, Poly(methylene oxide), POM 2560
Polystyrene, PS 16910
Polysulfone, PSU 2315
1The entanglement weights are the average of several experimental values.